What's the annealing time and temp, please? Thanks

Sharlyn
Technically for Boro, 10 mins. per millimeter thickness at 1050 degrees measured at the thickest point. You can probably just run the kiln up to 1050 and turn it off, let it come down on its own. At 500 degrees you can vent the kiln a bit and cool it down a bit faster.