Annealing schedule voor Moretti glas, it's in Celcius
Step 1: In 222 degrees/hour to a temperature of 521 degrees. Hold that temperature for about 30 minutes.
Step 2: In 45 degrees/hour nto a temperature of 454 degrees. Hold that temperature for about 15 minutes.
Stap 3: Kiln off.
In this book:
The Complete Book of Glass Beadmaking
from Kimberley Adams
There is a schedule in Fahrenheit.
__________________
Greetings from the Netherlands,
Margriet.